5 EXECUTION ON SITE
KFR-TDE0014483
5.1 Touch-up of degradation of coating
Surface preparation: derusting with mechanical brush as per PSt 2/PSt 3;
Grind by using abrasive paper with a granulation
ranging from 80 to 100. When doing so, create flat, soft
transfers towards the intact zone.
Whet once by using abrasive paper of a granulation
between 60 and 80.

Paint structure painting material Type of paint Application NDFT


manufacturers method / (µm)
Products
Prime coat Surface-tolerant brush / spray 100
System No. 1.1 2-pack epoxy
and 1.3
Hempel Hempadur Mastik 45880

International Interplus 256

Jotun Primastic universal

Prime coat see 3.1 brush / spray 3.1 +


all other systems 20µm
Intermediate coat see 3.1 brush / spray 120
/ roll
Finishing coat see 3.1 brush / spray 60
/ roll
Dry film thickness 280

5.2 Special items / special surfaces

5.2.1 Systematically pre-stressed connections (see 3.2.1)

5.2.1.1 Friction-grip connections


- - Wash off zinc salt from the still visible area of the prime coat by using water and sponge
(ScotchBrit). If need be, carry out a touch-up of the prime coat according to 5.1.
- Apply intermediate coat as per indication under 5.1. Take care to thickly apply the paint
materials in the zone of adjacent contact areas.
- Seal the broader joints with a permanently elastic sealing compound to be overpainted
(Sikaflex 221 or equivalent).
- Apply finishing coat according to the description under 5.1. Take care to thickly apply the